How-to · Beginner · 4 min read
How to Solder Electronics
Iron Temperature, Solder and Technique
By Geekobot Learning Team · Updated 24 Oct 2026
On this page
To solder a through-hole joint, heat the pad and component lead together with a clean, tinned iron for one to two seconds, feed solder into the joint (not onto the iron) until it flows into a small shiny cone, then remove the solder and the iron. Set about 330 to 350 °C for leaded solder and 350 to 380 °C for lead-free.
Key specs at a glance
- Iron
- Temperature-controlled, 40 to 80 W, chisel tip about 2 mm
- Solder
- 0.6 to 0.8 mm rosin-core; 63/37 or 60/40 leaded, or SAC305 lead-free
- Melting point
- 63/37: 183 °C; SAC305: about 217 to 220 °C
- Tip temperature
- Leaded about 330 to 350 °C; lead-free about 350 to 380 °C
- Essentials
- Stand, brass wool or damp sponge, flux, wick or pump, fume extraction
- Joint time
- About 2 to 3 seconds per joint
What you need to start soldering
Shop this list2 of 6 found in our store · ₹461
- Temperature-controlled iron or station: a fixed-power 25 W iron works for practice, but a controlled iron makes better joints and lasts longer.Find this part
- Solder: 0.8 mm rosin-core is easiest. Leaded (63/37) flows easily for learning; lead-free is required for many commercial products.Find this part
- Flux pen or paste: makes solder flow, essential for reworking and SMD.Find this part
Brass wool cleaner, stand, desoldering wick and pump.Desoldering Wick₹15
Helping hands or a PCB holder, side cutters and safety glasses.Helping Hands and PCB Holder₹446Closest match, check the specs- Practice kit: a soldering practice kit teaches technique on cheap parts.Find this part
Step-by-step: soldering a through-hole joint
- 1Tin the tip: melt a little solder onto the clean tip so it shines.
- 2Insert and bend: push the component lead through the hole and bend it slightly so it stays put.
- 3Heat both: touch the tip so it contacts both the pad and the lead for about one second.
- 4Feed solder: touch solder to the joint on the opposite side from the tip. It should melt and flow around the lead.
- 5Remove solder, then iron: stop feeding after about a second, then lift the iron away.
- 6Do not move it for a few seconds while it solidifies.
- 7Trim the lead just above the joint.
Good vs bad solder joints
| Joint | Looks like | Cause | Fix |
|---|---|---|---|
| Good | Smooth concave cone, shiny (leaded) or satin (lead-free) | ||
| Cold joint | Dull, grainy, lumpy | Not enough heat, or moved while cooling | Add flux and reheat |
| Blob | Ball sitting on top of the pad | Solder melted on the iron, pad not heated | Reheat pad and lead together |
| Bridge | Solder joining neighbouring pads | Too much solder | Drag with a clean tip and flux, or use wick |
| Dry pad | Solder on the lead but not the pad | Dirty or oxidised pad | Clean, add flux, reheat |
- Good
- Looks like:
- Smooth concave cone, shiny (leaded) or satin (lead-free)
- Cold joint
- Looks like:
- Dull, grainy, lumpy
- Cause:
- Not enough heat, or moved while cooling
- Fix:
- Add flux and reheat
- Blob
- Looks like:
- Ball sitting on top of the pad
- Cause:
- Solder melted on the iron, pad not heated
- Fix:
- Reheat pad and lead together
- Bridge
- Looks like:
- Solder joining neighbouring pads
- Cause:
- Too much solder
- Fix:
- Drag with a clean tip and flux, or use wick
- Dry pad
- Looks like:
- Solder on the lead but not the pad
- Cause:
- Dirty or oxidised pad
- Fix:
- Clean, add flux, reheat
How to desolder
- Desoldering pump: heat the joint until fully molten, place the pump nozzle on it, and trigger.
- Desoldering wick (braid): lay wick on the joint, press the iron on top, and the copper soaks up the solder. Add flux for best results.
- For multi-pin parts, cut the component free first, then remove each pin separately.
Soldering safety
The tip is hot enough to cause serious burns, so always return it to the stand. Work in a ventilated space or use a fume extractor; flux smoke irritates the lungs. Wash your hands after using leaded solder and do not eat at the bench. Wear glasses when trimming leads, which can fly off at speed.
Try it: Temperature converter: °C, °F, K
Change the values and the diagram and results update as you type.
Common mistakes to avoid
- Carrying solder to the joint on the iron tip; the flux burns off and the joint is poor.
- Not heating the pad, which leaves solder balled on the lead.
- Holding the iron on too long and lifting pads off the board.
- Letting the tip go black and untinned; clean and re-tin it often.
- Using plumbing solder or acid flux, which corrodes electronics.
Frequently asked questions
What temperature should a soldering iron be for electronics?
About 330 to 350 °C for leaded solder and 350 to 380 °C for lead-free. Use more for large ground planes and thick wires, less for small SMD parts.
Leaded or lead-free solder: which is better for beginners?
Leaded 63/37 solder melts at a lower temperature and flows more easily, which makes learning easier. Lead-free is safer for the environment and required for products sold in many markets.
What wattage soldering iron should I buy?
A temperature-controlled iron of 40 to 80 W recovers heat quickly. Cheap fixed 25 W irons are fine for occasional small joints but struggle with thick wires.
Why won't solder stick to my iron or the board?
The tip or pad is oxidised or dirty. Clean the tip on brass wool, re-tin it, and add flux to the joint.
Do I need flux if my solder has a rosin core?
For simple through-hole joints, the core is enough. Extra flux helps with reworking, desoldering, SMD parts and old or oxidised boards.
Parts for this guide
Terms in this guide
Keep learning
Sources
- IPC J-STD-001 requirements for soldered electrical and electronic assemblies
- Kester and Alpha solder alloy datasheets (63/37, SAC305)
Written by the Geekobot team from manufacturer datasheets. Always check the datasheet for the exact part and variant you buy.